SA299 GrA and A299 GrA steel are the same material, but the implementation standards are different. A299 GrA implements ASTM A299/A299M-04, SA299 GrA implements ASME SA-299/SA-299M-2015. The chemical composition and mechanical properties of SA299 GrA and A299 GrA steel are the same.
Mechanical properties of SA299 GrA and A299 GrA steel:
Delivery status | Thickness (mm) | Mechanical properties | ||
Hot rolled, normalized | >25-50 | Rp0.2(MPa) | ≥275 | |
Rm(MPa) | 515-655 | |||
A200(%) | ≥16 | A50≥19% | ||
Impact temperature | -1 | |||
Akv(J) | ≥20 | Longitudinal | ||
Bending diameter | 2.5a | |||
Bending angle | 180 | |||
>50-75 | Rp0.2(MPa) | ≥275 | ||
Rm(MPa) | 515-655 | |||
A200(%) | ≥16 | A50≥19% | ||
Impact temperature | -1 | |||
Akv(J) | ≥20 | Longitudinal | ||
Bending diameter | 3a | |||
Bending angle | 180 | |||
>75-125 | Rp0.2(MPa) | ≥275 | ||
Rm(MPa) | 515-655 | |||
A200(%) | ≥16 | A50≥19% | ||
Impact temperature | 4 | |||
Akv(J) | ≥20 | Longitudinal | ||
Bending diameter | 3a | |||
Bending angle | 180 |
Smelting Analysis of chemical composition of SA299 GrA and A299 GrA steel:
C | Si | Mn | P | S | Ni | Cr | Mo | Cu | Nb | V | Ti | Alt | B |
≤0.28 | 0.15-0.4 | 0.9-1.5 | ≤0.025 | ≤0.025 | ≤0.4 | ≤0.3 | ≤0.12 | ≤0.4 | ≤0.02 | ≤0.03 | ≤0.03 | ≥0.02 | ≤0.001 |
Remarks for composition: Cr+Ni+Mo+Cu≤0.03; Cr+Mo≤0.32; Als can be used instead of Alt, at this time Als≥0.015.